Iron Copper and Copper Steel
| Material | Chemical Composition, % |
In-House Material Code Specification |
MPIF Equivalent Specification |
Density (G/cc) |
Ultimate Tensile Strength |
Yield Strength (PSI) |
Elongation % in one inch |
Macro Apparent Hardness Rockwell Scale |
Micro Converted Hardness Rockwell Scale |
Application |
| Copper Iron | Iron: 93.8 - 98.5 Copper: 1.5 - 3.9 Max Carbon: 0.0 - 0.3 Max Other: 0.2 Max |
CS 0970 F | FC-0200-15 FC-0200-18 FC-0200-21 FC-0200-24 |
6.0 6.3 6.6 6.9 |
25,000 28,000 31,000 34,000 |
20,000 23,000 26,000 29,000 |
1.0 1.5 1.5 2.0 |
10HRB 18HRB 26HRB 36HRB |
N/A | Mechanical components requiring low to medium strength and good bearing quality iron with copper. Excellent for oil impregnation. |
| Copper iron | Iron: 87.2 - 98.2 Copper: 9.5 - 10.5 Max Carbon: 0.0 - 0.3 Max Other: 2.0 Max |
CS 9001 | FC-1000-20 | 6.0 | 30,000 | 26,000 | <1.0 | 15HRB | N/A | Mechanical components requiring low to medium strength and good bearing quality iron with copper. Excellent for oil impregnation. |
| Copper Steel Low Carbon | Iron: 93.5 - 98.2 Copper: 1.5 - 3.9 Max Carbon: 0.3 - 0.6 Max Other: 2.0 Max |
CS 0975 FS | FC-0205-30 FC-0205-35 FC-0205-40 FC-0205-45 |
6.0 6.3 6.7 7.0 |
35,000 40,000 50,000 60,000 |
35,000 40,000 45,000 50,000 |
<1.0 <1.0 <1.0 <1.0 |
37HRB 48HRB 60HRB 72HRB |
N/A | Mechanical components requiring medium to good strength and bearing quality iron with copper. Excellent wear capabilities. |
| Copper Steel Low Cabon Heat Treated | Iron: 93.5 - 98.2 Copper: 1.5 - 3.9 Max Carbon: 0.3 - 0.6 Max Other: 2.0 Max |
CS 0975 FS (HT) |
FC-0205-60HT FC-0205-70HT FC-0205-80HT FC-0205-90HT |
6.2 6.5 6.8 7.0 |
70,000 80,000 90,000 100,000 |
70,000 80,000 90,000 100,000 |
<0.05 <0.05 <0.05 <0.05 |
19HRC 25HRC 31HRC 36HRC |
58HRC 58HRC 58HRC 58HRC |
Mechanical components requiring medium to good strength and bearing quality iron with copper. Excellent wear capabilities. |
| Copper Steel High Carbon | Iron: 93.2 - 97.9 Copper: 1.5 - 3.9 Max Carbon: 0.6 - 0.9 Max |
CS 0972 FS | FC-0208-30 FC-0208-40 FC-0208-50 FC-0208-60 |
5.8 6.3 6.7 7.2 |
35,000 50,000 60,000 70,000 |
35,000 45,000 55,000 65,000 |
<1.0 <1.0 <1.0 <1.0 |
50HRB 61HRB 73HRB 84HRB |
N/A | Mechanical components requiring good to higher strength and bearing quality iron with copper. Excellent wear capabilities. |
| Copper Steel High Carbon Heat Treated | Iron: 93.2 - 97.9 Copper: 1.5 - 3.9 Max Carbon: 0.6 - 0.9 Max Other: 2.0 Max |
CS 0972 FS (HT) |
FC-0208-50HT FC-0208-65HT FC-0208-80HT FC-0208-95HT |
6.1 6.4 6.8 7.1 |
65,000 75,000 90,000 105,000 |
65,000 75,000 90,000 105,000 |
<0.05 <0.05 <0.05 <0.05 |
20HRC 27HRC 35HRC 43HRC |
60HRC 60HRC 60HRC 60HRC |
Mechanical components requiring good to higher strength and bearing quality iron with copper. Excellent wear capabilities. |
| Copper Steel High Carbon | Iron: 91.4 - 95.7 Copper: 4.0 - 6.0 Max Carbon: 0.3 - 0.6 Max Other: 2.0 Max |
CS 9505 FS | FC-0505-30 FC-0505-40 FC-0505-50 |
5.8 6.3 6.7 |
44,000 58,000 71,000 |
36,000 47,000 56,000 |
<0.05 <0.05 <1.0 |
51HRB 62HRB 72HRB |
N/A | Mechanical components requiring good to higher stength and bearing quality iron with copper. Excellent wear capabilities. |